Reading GB/T 699: What the Grade Number Tells You Before You Quote
A drawing arrives marked "45#". The part is a shaft, 60 mm at the bearing seat, hardened and tempered. Nothing else on the drawing says what the steel is. This article is about that moment: how the Chinese carbon steel designation system works, what the two-digit number actually measures, and where the designation stops telling you anything useful.
GB/T 699 is the Chinese standard for quality carbon structural steel. It is the direct counterpart of the general-purpose carbon steels used across Europe and North America, and in most shaft, pin, sleeve and general mechanical work it is interchangeable with them. The differences that matter are the phosphorus and sulphur limits, the availability of the manganese grades, and the fact that the number in the grade name is a carbon content rather than a sequence number.
What "Quality" Adds Over Ordinary Carbon Steel
Chinese standards separate ordinary carbon structural steel from quality carbon structural steel, and the split is about impurity control, not strength. Both families contain grades at the same carbon level. The quality grades carry tighter limits on phosphorus and sulphur, and that difference shows up in toughness, fatigue life and how predictable the steel is after heat treatment.
| Family | Standard | Typical P and S limits | What it means in practice |
|---|---|---|---|
| Quality carbon structural steel | GB/T 699 | P ≤ 0.035%, S ≤ 0.035% | Used for machined mechanical parts, shafts, gears, fasteners that will be heat treated. |
| Ordinary carbon structural steel | GB/T 700 | P ≤ 0.045%, S ≤ 0.050% | Used for structural sections, welded frames, general fabrication. Not normally chosen for a hardened, fatigue-loaded machined part. |
The practical consequence is that a Q235 plate and a 20 round bar are not interchangeable even though both are low-carbon steels. If a drawing specifies 45#, substituting an ordinary carbon steel at the same carbon level is a non-conformance on cleanliness grounds, not on strength grounds, and it is the kind of substitution that passes dimensional inspection and then fails a fatigue test.
The Grade Number Is the Carbon Content
The rule is simple and it holds for the whole series: the number is the nominal carbon content in hundredths of a percent. Grade 45 means 0.45% carbon. Grade 20 means 0.20%. Grade 08 means 0.08%.
Once you know that, the family reads as a continuous ladder of carbon content, and almost every property difference follows from it. Carbon raises hardness and strength potential, and it lowers ductility, weldability and machinability in the annealed condition. Everything else in the table below is a range around that single number.
Two details are worth knowing because they cause misreads. First, the number is nominal: actual carbon sits in a range around it, typically plus or minus 0.04%, and the mill certificate is the authoritative figure. Second, the manganese grades use the same number for carbon and add Mn to the designation, so 45Mn is not a higher-carbon version of 45 — it is 45 with more manganese.
The Six Elements, and What Each One Is Doing
| Element | Typical range | Function | What goes wrong at the limit |
|---|---|---|---|
| C — carbon | 0.05–0.90% depending on grade | Sets hardness, strength and hardenability potential | Too high for the application: ductility, weldability and machinability fall away |
| Si — silicon | 0.17–0.37% | Deoxidation during steelmaking; mild strength contribution | Rarely a problem at these levels; not a hardening element here |
| Mn — manganese | 0.35–1.00% | Improves hardenability and strength; ties up sulphur to reduce hot shortness | Higher Mn means higher hardenability, which changes the heat-treat response even at identical carbon |
| P — phosphorus | ≤ 0.035% | Treated as a residual impurity | Raises cold brittleness and lowers toughness; the main reason quality grades cost more |
| S — sulphur | ≤ 0.035% | Treated as a residual impurity in these grades | Hot shortness during forging or rolling; in machining grades S is added deliberately, which is a different product |
| Cr, Ni, Cu | Residual, capped | Not intentional alloying in this family | A residual Cr or Ni reading does not make the steel an alloy steel; check the designation, not the certificate |
The Grades, From 08 to 85
Silicon is 0.17–0.37% and phosphorus and sulphur are each ≤ 0.035% for every grade in this table unless stated otherwise. Manganese changes with carbon level, which is why it is shown.
| Grade | C (%) | Mn (%) | Character | Where it is normally used |
|---|---|---|---|---|
| 08 | 0.05–0.11 | 0.35–0.65 | Very low carbon, high ductility, low strength | Cold-formed and stamped parts, thin sheet components, low-load panels |
| 10 | 0.07–0.13 | 0.35–0.65 | Good ductility, toughness and weldability | Small shafts, pins, sleeves, welded and cold-headed parts |
| 15 | 0.12–0.18 | 0.35–0.65 | Low carbon with toughness, suitable for case hardening | Small gears, bushings, pins, low-load components |
| 20 | 0.17–0.23 | 0.35–0.65 | The default low-carbon machine steel; weldable and case hardenable | Shafts, pins, sleeves, bolts, sprockets, carburised parts |
| 25 | 0.22–0.29 | 0.50–0.80 | Stronger than 20 with usable ductility | Shafts, pins, bolts, general mechanical parts |
| 35 | 0.32–0.39 | 0.50–0.80 | Balanced strength and toughness | General shafts, tie rods, connecting rods, fasteners |
| 40 | 0.37–0.44 | 0.50–0.80 | Higher strength, responds to normalising and quenching and tempering | Shafts, gears, connecting rods, transmission parts |
| 45 | 0.42–0.50 | 0.50–0.80 | The most common medium-carbon machine steel | Shafts, gears, pins, sleeves, crankshafts, transmission parts |
| 50 | 0.47–0.55 | 0.50–0.80 | Higher strength and hardness, lower toughness | Wear parts, elastic parts, shafting |
| 55 | 0.52–0.60 | 0.50–0.80 | High strength and hardness, poor weldability | Springs and elastic parts, wear parts, shims |
| 60 | 0.57–0.65 | 0.50–0.80 | High strength, good elasticity and wear resistance | Spring plates, wear parts, shims |
| 65 | 0.62–0.70 | 0.50–0.80 | High carbon, high hardness, limited ductility | Elastic parts, wear parts, simple tooling |
| 70 / 75 / 80 / 85 | 0.67–0.90 | 0.50–0.80 | High carbon, high hardness and wear resistance, low toughness | Spring strip, wear plates, simple cutting and forming tools |
The Mn Series: Same Carbon, More Hardenability
Above roughly 0.60% manganese the designation picks up "Mn", and the carbon range stays where it was. Manganese at 0.70–1.00% instead of 0.35–0.80% does two things: it raises hardenability, so a larger section can be through-hardened, and it raises strength slightly in the as-supplied condition. It does not make the steel an alloy steel in the GB/T 3077 sense, and it does not change the fact that the carbon level still governs the achievable hardness.
| Grade | C (%) | Mn (%) | Compared with the base grade |
|---|---|---|---|
| 15Mn | 0.12–0.18 | 0.70–1.00 | Better strength and hardenability than 15; still a case-hardening candidate |
| 20Mn | 0.17–0.23 | 0.70–1.00 | Higher strength and better heat-treat response than 20 |
| 25Mn | 0.22–0.29 | 0.70–1.00 | Stronger than 25 for general load-bearing parts |
| 30Mn / 35Mn | 0.27–0.39 | 0.70–1.00 | Better strength and hardenability than 30 and 35 |
| 40Mn / 45Mn | 0.37–0.50 | 0.70–1.00 | Respond well to quenching and tempering in larger sections than 40 or 45 |
| 50Mn and above | 0.47–0.62 | Higher than the base grade | More strength, hardness and wear resistance; less toughness |
The Mn series is where substitution gets risky. A buyer who reads "20Mn" as "20 with a bit more manganese" and orders 20 will get a part that is dimensionally correct and shallower-hardening than the drawing assumed. When the drawing calls for a Mn grade, the grade is the requirement.
Selecting by the Job, Not by the Number
| Requirement | Grades normally considered | Why |
|---|---|---|
| Cold forming, stamping, thin sections | 08, 10 | Lowest carbon, highest ductility |
| Welded assemblies and low-load parts | 10, 15, 20 | Toughness and weldability |
| Case-hardened small gears, bushings, pins | 15, 20, 20Mn | Low core carbon allows a hard case over a tough core |
| General shafts, pins, sleeves, tie rods | 35, 40, 45 | Balanced strength and toughness |
| Quenched and tempered shafts and transmission parts | 40, 45, 40Mn, 45Mn | Good response to quenching and tempering |
| Gears, connecting rods, loaded parts | 45, 20Mn, 25Mn, 40Mn | Higher strength and hardenability |
| Springs, shims, wear plates | 60, 65, 70, 65Mn | Hardness, elasticity and wear resistance |
What a Drawing Marked 45# Means Outside China
For the common grades there is a close European and American counterpart, and for most machined parts the substitution is safe. The carbon and manganese ranges line up; the differences sit in the residual element limits and in what the mill actually certifies.
| GB/T 699 grade | Closest EN designation | AISI / SAE | JIS |
|---|---|---|---|
| 10 | C10 | 1010 | S10C |
| 15 | C15 | 1015 | S15C |
| 20 | C22 | 1020 | S20C |
| 25 | C25 | 1025 | S25C |
| 35 | C35 | 1035 | S35C |
| 40 | C40 | 1040 | S40C |
| 45 | C45 | 1045 | S45C |
| 50 | C50 | 1050 | S50C |
| 55 | C55 | 1055 | S55C |
| 60 | C60 | 1060 | S60C |
| 65 | C65 | 1065 | S65C |
| 20Mn | 20Mn5 | 1022 (higher Mn) | SMn420 |
These are close, not identical. The EN equivalents carry their own residual limits and their own hardenability bands, and the manganese grades in particular have no complete European series. Where the part is fatigue-loaded, quenched and tempered, or specified with a hardness at a stated depth, the certificate should be checked against the drawing rather than against a substitution table.
What to Put in an RFQ for a Carbon Steel Part
- The grade as it appears on the drawing, including the Mn suffix if there is one, and the standard if the drawing names one.
- The delivery condition: hot rolled, normalised, annealed, or quenched and tempered to a stated hardness range.
- Whether final machining happens before or after heat treatment, and how much stock is left for grinding if any.
- Any hardness, tensile or case-depth requirement, and where on the part it is measured.
- The certificate level required, and whether a 3.1 or 3.2 inspection document is expected.
- Whether the drawing assumes a European or American grade and has been translated, since a translated drawing sometimes carries a grade that does not exist in the original standard.
Frequently Asked Questions
Is 45# steel the same as C45?
Close enough for most machined parts, and different on paper. Both sit at 0.42–0.50% carbon with 0.50–0.80% manganese, so the mechanical behaviour after quenching and tempering is essentially the same. The residual element limits and the certified hardenability band are set by different standards, so a part specified with a hardness at depth should be verified against its own certificate rather than treated as interchangeable.
Why does the drawing say 45# rather than a grade number?
The "#" is a Chinese shorthand for "steel" that survived from older drawing practice, so 45# and 45 mean the same grade. It is common on drawings produced in China for domestic production and then sent abroad with a part. It is a designation, not a grade of its own, and it does not imply a particular delivery condition.
Can a higher-carbon grade replace a lower one to get more strength?
Usually not without other changes. Moving from 45 to 50 raises achievable hardness, and it also reduces ductility, toughness and weldability, and it makes the part more sensitive to quench cracking in thin sections or at sharp transitions. Where strength is short, the usual routes are a different heat-treat condition, a larger section, or an alloy grade, and each of those needs to be decided before the drawing is released.
Need a Carbon Steel Component Machined?
DXSCNC machines drawing-based carbon and alloy steel components: shafts, pins, sleeves, bushings, threaded parts and flanged bodies, in the condition the drawing specifies.
Use the model-specific machining limits when planning a part. Material, geometry, tolerance, workholding and inspection affect machine selection.
Related DXSCNC resources: 45# Steel CNC Machining, When 45# Steel Is Not Enough, 42CrMo4 CNC Machined Parts, CNC Turning and Quality Inspection.